Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® Advanced T1000HG10 LS BK - PA6T/6I-GF50 - BASF

Material Data Center offers the following functions for Ultramid® Advanced T1000HG10 LS BK:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Heat stabilized, partially aromatic polyphthalamide for injection molding with strong mechanical properties especially at elevated temperatures, and excellent chemical resistance for highly stressed parts. Ultramid® Advanced T1000HG10 LS BK can be characterized as compound with high strength and stiffness, very low water absorption and outstanding dimensional stability. It features a high melting point (320°C) and excellent melt stability.

Markets & applications
Automotive: Fuel system, cooling system, powertrain, metal replacement
Industry goods: Pumps, compressors
Consumer goods: Home appliances, consumer electronics, furniture fittings
Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Retrait au moulage, parallèle 0.5 / * % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 0.9 / * % ISO 294-4, 2577
Propriétés mécaniquessec / condUnitéNorme du test
ISO Data
Module en traction 18000 / 18000 MPa ISO 527
Contrainte à la rupture 250 / 250 MPa ISO 527
Déformation à la rupture 1.8 / 1.8 % ISO 527
Résistance au choc Charpy, +23°C 75 / 70 kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C 65 / 65 kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 10 / 11 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), -30°C 10 / 10 kJ/m² ISO 179/1eA
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 320 / * °C ISO 11357-1/-3
Température de fléchissement s/chrg, 1.80 MPa 280 / * °C ISO 75-1/-2
Propriétés électriquessec / condUnitéNorme du test
ISO Data
Résistivité transversale - / >1E13 Ohm*m IEC 62631-3-1
Résistivité superficielle * / >1E15 Ohm IEC 62631-3-2
Rigidité diélectrique 40 / - kV/mm IEC 60243-1
Indice de résistance au cheminement - / 550 - IEC 60112
Propriétés diversessec / condUnitéNorme du test
Absorption d'eau 2.9 / * % Sim. to ISO 62
Absorption d'humidité 1.3 / * % Sim. to ISO 62
Masse volumique 1640 / - kg/m³ ISO 1183
Propriétés spécifiques à la matièresec / condUnitéNorme du test
ISO Data
Indice de viscosité 100 / * cm³/g ISO 307, 1157, 1628
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 350 °C ISO 294
Injection, température du moule 150 °C ISO 294
Fonctions
Module de cisaillement dynamique / Température , Ultramid® Advanced T1000HG10 LS BK (sec), PA6T/6I-GF50, BASF
Module de cisaillement dynamique / Température , Ultramid® Advanced T1000HG10 LS BK (cond.), PA6T/6I-GF50, BASF
Contrainte / Déformation , Ultramid® Advanced T1000HG10 LS BK (sec), PA6T/6I-GF50, BASF
Contrainte / Déformation , Ultramid® Advanced T1000HG10 LS BK (cond.), PA6T/6I-GF50, BASF
Module sécant / Déformation , Ultramid® Advanced T1000HG10 LS BK (sec), PA6T/6I-GF50, BASF
Module sécant / Déformation , Ultramid® Advanced T1000HG10 LS BK (cond.), PA6T/6I-GF50, BASF
Module de traction / Température , Ultramid® Advanced T1000HG10 LS BK (sec), PA6T/6I-GF50, BASF
Module de traction / Température , Ultramid® Advanced T1000HG10 LS BK (cond.), PA6T/6I-GF50, BASF
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés, Noir
Propriétés spéciales
Stabilisé à la chaleur
Caractéristiques
Tenue de la matière à l’état fondu
Résistance Chimique
Résistance chimique générale
Applications
Automobile, Électrotechnique et électrique
Disponibilité régionale
Autres informations
Moulages par injection
PREPROCESSING
Pre/Post-processing, max. allowed water content: .05 %
Pre/Post-processing, Pre-drying, Temperature: 120 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 345 - 355 °C
injection molding, Melt temperature, recommended: 350 °C
injection molding, Mold temperature, range: 150 - 190 °C
injection molding, Mold temperature, recommended: 150 °C
injection molding, Dwell time, thermoplastics: 5 min
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.